Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the js_composer domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /var/www/wp-includes/functions.php on line 6121

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the salient domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /var/www/wp-includes/functions.php on line 6121
Plastic Injection - Pre Hardened V'1.2085 - V Steels Skip to main content

Plastic Injection

– Pre Hardened –

Industeel 1.2085

A resulfurized prehardened (300HB) and corrosion resistant mould steel

Chemical Properties

NO DIN C Si Mn P S Cr Ni
V'1.2085 X33Cr16+S 0.33 0.3 1.10 Max 0,03 Max 0,07 16.00 1.0

Material Propeeties

  • Very good corrosion resistance.
  • Very Good machinability.
  • Magnetizable steel.
  • Very good for operating in wet and corrosive environments.
  • Very good dimensional stability during heat treatment.
  • Not designed for highly polished and etched surfaces

Applications

This steel is commonly used for mould steel applications including holders or support plates subjected to wet working and/or storage conditions. The grade is also used for the manufacturing of corrosive materials like PVC.

  • Mold plates, frames and holders
  • Support plates.
  • Manufacturing of corrosive materials like PVC.
  • Dies and die blocks in the plastics industry,
  • Rubber Molds.
  • Machinery parts requiring corrosion resistance.

Heat Treatment

Recomended to use as prehardened.

Physical Properties

Thermal Conductivity W.m-1.K-1 Thermal Expansion Coefficient (10-6.K-1)
20 °C 20-100 20-200 20-300 20-400 Specific heat J/kg °C
24,3 11 11,1 11,4 11,7 460
Hardness Rp 0.2 Yield strength Rm Tensile strength Elongation Contraction Elastic Modulus
HB MPa MPa % % GPa
320 905 1100 10 21 207

Delivery Condition

Prehardened, 280-325 HB (29-33 HRC).