Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the js_composer domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /var/www/wp-includes/functions.php on line 6121

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the salient domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /var/www/wp-includes/functions.php on line 6121
Aluminum Extrusion 1.2343 VEXtra - V Steels Skip to main content

Aluminum Extrusion

1.2343 VEXtra

Hot work tool steel with ESR properties. Good combination of toughness and hot strength.

Chemical Composition

NO DIN C Si Mn P S Cr Mo V
1.2343 VEXtra X37CrMoV5-1 0,33-0,41 0,80-1,20 0,25-0,50 Max 0,025 Max 0,008 4,80-5,50 1,10-1,50 0,30-0,50

Material Properties

  • Good toughness and ductility.
  • Good enough hot strength and tempering back resistance.
  • Good cleanness and homogeneity.
  • Good Polishability.
  • Good for texturing.
  • Good weldability.
  • Good machinability.
  • Up to 54 HRc after the heat treatment.
  • Recommended working hardness 44-52 HRc.
  • Good nitriding and coating ability.
  • Good thermal conductivity.

Applications

  • All press forging dies and cores
  • Precision Plastic injection molds
  • Molds for abrasive polymers and reinforced resins
  • Low pressure die casting dies
  • High pressure die casting dies
  • Industrial knives & blades resistant to cracking and breaking
  • Punches, cutting and shearing blades thicker than 10 mm.

Heat Treatment

HEAT TREATMENT TEMPERATURE
Soft Annealing 750-800°C
Stress Relieving 600-650°C
Hardening 1020-1060°C
Tempering 530-700°C

Physical Properties

20°C 100°C 400°C 500°C 600°C
Elastic Modulus [kN/mm²] 210 - 183 176 168
Thermal Expansion Coefficient [10ˉ6/K] - 10,7 11,8 11,9 12,4
Thermal Conductivity [W/mK] - 28,4 27,1 29,9 28,5

Delivery Condition

230 HB, Soft Annealed.

Tempering Graph